Corrosion Allowance on Dished Heads: Why Copying the Shell Number Fails
Corrosion allowance for a pressure vessel is written as a single number on the drawing. Most buyers carry it across from the shell without questioning it, and on a dished head that number is only one of three deductions. The other two happen before the head leaves the shop: the mill rolls plate slightly under nominal, and forming pulls the wall thinner at the knuckle. Stack them in the wrong order and the head can sit below its design thickness on the day it arrives, with no corrosion yet.
What the code says, and what it does not
UG-25 is a short paragraph. It requires corrosion to be addressed; it does not hand out a value. The number comes from the design basis - expected metal loss per year multiplied by design life, or the owner company's specification, whichever governs. Any article stating that ASME requires 3 mm on every vessel is describing a habit, not a rule.
The 1/16 inch figure that circulates widely has a real source, and it is narrower than most people think. 46 CFR 54.01-35 is a U.S. Coast Guard rule for vessels under its jurisdiction, and it explicitly modifies UG-25. It sets the allowance at one-sixth of the calculated thickness or 1/16 inch, whichever is smaller, added to the calculated thickness, and it releases the requirement where the effective stress stays at or below 80 percent of the allowable. That is a marine rule for a defined fleet. Copying it onto a chemical reactor in another jurisdiction is a coincidence dressed up as compliance.
What the code does fix is the geometry. UG-27 defines R as the inside radius in the corroded condition, and the reason is physical: corrosion grows the radius from the inside, and hoop stress rises with radius. Designing on the new, uncorroded radius produces a wall that is already thin at the end of its life. UG-32 works on the inside diameter, and the same convention follows. The allowance therefore enters the calculation twice - once as metal added to the required thickness, and once as a larger diameter inside the formula.
Three quantities, not one
The confusion starts when these are treated as the same kind of number. Two of them are thickness you need. Two of them are thickness you will lose, at different times and for different reasons.
|
Quantity |
Where it comes from |
Typical size |
Who carries the risk |
|
Design thickness t |
UG-32 formula on the corroded diameter |
3–20 mm |
Designer |
|
Corrosion allowance c |
Design basis: rate × life, or owner spec |
Often 0–6 mm |
Owner and designer |
|
Forming thinning |
0.5–2 mm on a 10–20 mm plate |
Manufacturer |
|
|
Mill under-tolerance |
Plate standard, permitted up to 0.25 mm or 6% of ordered thickness |
Up to 0.25 mm |
Mill and buyer |
The first two are decided at the desk. The last two are decided in the rolling mill and under the press. A purchase order that names only the first two leaves the other two to chance.
The sequence that works
Take a 2:1 elliptical head, 1000 mm inside diameter in the corroded condition, design pressure 1.0 MPa, allowable stress 138 MPa, joint efficiency 1.00. The numbers below are an arithmetic demonstration, not a substitute for a design calculation.
|
Step |
What you do |
Result |
|
1 |
Design thickness on the corroded diameter: t = PD / (2SE − 0.2P) |
3.63 mm |
|
2 |
Add the allowance: t required after forming = t + c, with c = 3 mm |
6.63 mm |
|
3 |
Gross up for forming thinning: nominal ≥ 6.63 / (1 − 0.10) |
7.36 mm |
|
4 |
Select plate: 8 mm, then check mill under-tolerance is inside the permitted band |
8 mm ordered |
|
5 |
Verify after forming: 8 × 0.90 = 7.20 mm; 7.20 − 3.00 = 4.20 mm against 3.63 mm |
Passes with 0.57 mm spare |
Now run the same head with c = 4 mm and keep the 8 mm plate, because the shell beside it is 8 mm. After forming the wall measures 7.20 mm. Subtract the 4 mm the owner intends to lose over twenty years, and 3.20 mm is left to hold pressure. The design thickness is 3.63 mm. The head is 0.43 mm under at the knuckle before its first day in service, and no inspection at goods-in will call it a corrosion problem, because nothing has corroded.
The correct order for c = 4 mm is (3.63 + 4.00) / 0.90 = 8.47 mm, which means a 10 mm plate. Run the same arithmetic at 12 percent thinning on the 8 mm plate and the margin disappears faster: 7.04 mm after forming, 3.04 mm left with c = 4 mm. Both failures come from one decision - treating the shell thickness as the head thickness.

Why the head is not the shell
A shell course is rolled plate. It is bent to a radius, but its wall is not stretched over a tight transition, so the thickness that leaves the mill is close to the thickness that enters service. The allowance can be added to the plate and the arithmetic is short.
A head starts as a flat plate and becomes a curved surface with a knuckle. That knuckle is the tightest radius on the part and it takes the highest forming strain. The wall there is thinner than the plate that was ordered, always, and the reduction is a property of the process rather than a defect. So the starting point for a head is not shell plate plus allowance. It is design thickness plus allowance, divided by the fraction that survives forming.
There is a second, quieter difference. Heads are frequently ordered by inside diameter, and the inside surface is the one that corrodes. A shell ordered by outside diameter and a head ordered by inside diameter do not describe the same wall, and a specification that mixes the two conventions can shift the calculated thickness by a millimetre or more before anyone notices.
One number, but not one rate
The drawing carries a single allowance, and the corrosion it represents is rarely uniform across the part. In a horizontal vessel, the lower half of the head holds liquid and the upper half sees vapour; the liquid line between them is often the worst band on the whole closure, because it wets and dries and concentrates salts. In vertical service the bottom head collects solids and the top head collects condensate, and neither resembles the other.
A single figure is a practical compromise, and it is the right one for mild service. Where the mechanism is aggressive, thickening is a poor substitute for selection. Doubling the allowance buys time proportional to the extra metal, while pitting, crevice attack and chloride stress corrosion crack at a rate that wall thickness does not control. The cheaper answer is often a better grade, a lining, or a change in the process, and the more expensive answer is a heavier head that still fails in the same place.
Stainless steel with a zero allowance
Austenitic stainless heads are commonly specified with c = 0, and for uniform corrosion that is defensible: the general metal loss rate in most process streams is low enough that a design life passes without measurable wall loss. The mistake is reading zero as a statement about all corrosion.
Pitting, crevice corrosion and chloride stress corrosion cracking are localized mechanisms. They take a wall out through a small area, not across the surface, so extra thickness delays the event without preventing it. A 316L head in a chloride-bearing stream at 60 °C does not become safe by adding 3 mm; it becomes safe by moving to 2205, 904L or a 6Mo grade, or by bringing the chloride level and the temperature under control. The allowance is the wrong tool for that job, and a zero on the drawing is not a warranty.
What to check when the head arrives
Thickness readings by location, compared with design thickness plus allowance - not with the nominal plate thickness. A report that compares 7.2 mm with 8 mm proves nothing about the design.
The U-2A data report. The heads section carries two separate columns, minimum thickness and corrosion allowance. Read both, and confirm that the minimum thickness quoted is the formed thickness, not the plate ordered.
The mill certificate, for actual plate thickness against nominal, so the permitted under-tolerance is accounted for rather than discovered later.
The forming record, giving nominal plate before forming and measured minimum after. The difference is the real thinning for that shop and that process, and it is more useful than a catalogue range.
The inside diameter, measured after forming. If the head was ordered by ID, confirm that ID is what was measured, and that the allowance was applied to the corroded diameter.
Four mechanisms, and whether more wall helps
|
Mechanism |
Does extra wall help? |
Better response |
|
Uniform thinning - acid, condensate, mild process streams |
Yes. This is what the allowance is for. |
Set c from measured rate × design life, then gross up for forming |
|
Pitting and crevice attack |
Only delays it. The pit depth rate is unchanged. |
Grade upgrade, chloride control, surface finish, inspection interval |
|
Chloride stress corrosion cracking |
No. It is a stress and environment problem. |
Material change, stress relief, temperature and chloride limits |
|
Erosion-corrosion - slurry, high velocity |
Partly, and at a cost in weight and flow. |
Velocity limits, geometry, harder alloy |
Write the requirement into the order
An order that states a corrosion allowance on a dished head without saying where it is measured invites a head that meets the drawing and not the design. This wording closes that gap:
Head: 2:1 elliptical, seamless, ASME VIII Div. 1;
inside diameter 1000 mm in the corroded condition;
design thickness 3.63 mm per UG-32 at the stated design pressure;
corrosion allowance 3 mm, added to the design thickness;
minimum thickness after forming 6.63 mm at any point on the head;
plate nominal thickness selected by the manufacturer to guarantee
6.63 mm after forming, including permitted mill under-tolerance;
thickness measured at crown, knuckle (four meridians) and straight
flange, recorded by location; inside diameter verified after forming.
Dished heads and wall thickness at Dalian Dingjin
We form elliptical, torispherical and hemispherical heads in carbon steel and stainless steel, from two production bases and one R&D center in Dalian, and have supplied pressure vessel closures for more than 24 years. The plant holds a third-class pressure vessel manufacturing license and fabricates to ASME and other cited codes. Plate is checked for chemistry, mechanical properties and thickness before it enters production, each formed head is measured after forming with the wall recorded by location, and since 2014 we have shipped an average of more than 1,000 tons of dish heads a year.
FAQ
Q: Is there a standard corrosion allowance in ASME VIII-1?
A: No universal value. UG-25 requires corrosion to be addressed, and the amount comes from the design basis - expected rate over design life, or the owner specification. The 1/16 inch figure often quoted comes from 46 CFR 54.01-35, a U.S. Coast Guard rule that modifies UG-25 for vessels under its jurisdiction, not a general ASME requirement.
Q: Why is the allowance applied to the inside diameter or radius?
A: Because corrosion removes metal from the inside, which enlarges the radius, and hoop stress rises with radius. UG-27 defines R as the inside radius in the corroded condition for that reason. Designing on the new radius gives a wall that is already thin at end of life. UG-32 follows the same convention on the inside diameter.
Q: Can I use the same allowance on the head as on the shell?
A: The value can be the same; the arithmetic cannot. A shell keeps close to its rolled thickness, while a head loses 5 to 12 percent at the knuckle during forming. The head plate has to be selected as design thickness plus allowance, divided by the fraction that survives forming - which is normally one to two millimetres thicker than the shell plate.
Q: Does the corrosion allowance count toward MAWP?
A: No. The allowance is thickness intended to disappear during service, so it cannot also be counted as permanent pressure capacity. The ASME MAWP provisions, as reproduced in 46 CFR 54.10-5, exclude the specified corrosion allowance when the maximum allowable pressure is determined.
Q: Is a zero corrosion allowance acceptable on stainless steel?
A: Often yes for uniform corrosion, because the general loss rate is low. It is not a statement about pitting, crevice attack or chloride stress corrosion cracking, which are localized and are not controlled by wall thickness. Those need grade selection, chloride and temperature limits, and surface condition rather than extra metal.